HN-M92 Semi-Bright Nickel Plating
Commodity Name
HN-M92 Semi-Bright Nickel Plating
Composition and Working Conditions

 

Nickel sulfate

Nickel chloride

Boric acid    

Softener HN –M91

Leveler HN –M92

Stabilizer HN –M93  

Wetting agent HN -17

Temperature

pH value

Current density

Agitation

Filtration

Consumption:

Softener  HN –M91

Leveler HN –M92

Stabilizer  HN –M93

240~300g/L          

45~55g/L

40~50g/L    

4~6mL/L

0.4-0.6mL/L

0.4~0.6mL/L

1~2mL/L

45~55℃

4.0~4.8

2~6 A/dm2

Air agitation or mechanical agitation

Continuous cycle filtration

 

40~60 mL/1000A.H

100~150mL/1000A.H

30~50 mL/1000A.H

 

Application and Advantage

 

1. The sulfur content in deposit is less than 0.003%. Potential difference between semi-bright nickel layer 

and bright nickel layer is 120~145 mV. The corrosion resistance of deposit is excellent.

2. Good flexibility, excellent leveling and covering power & throwing power.

3. Strong concentration of additives, low consumption.

4. No coumarin in the bathe, less decomposed products, the plating bath is stable and is easy to control.